Prototype
Also called: Binder jetting, Sand printing
3D sand printing builds mould or core layer by layer from sand and binder. A core box is not needed. Undercuts that would need several cores in series can be one piece in the print. At Röth the process sits in Rapid prototyping, not as a substitute for the moulding line in series. That is binder jetting, not melting metal in the printer.
More … Rapid prototypingSand coreCore assembly
Rapid prototypingRequest advice
Standards
Also called: AD 2000, AD 2000 data sheet W0, AD 2000 W3/1, AD 2000 W3/2
AD2000 is a German code for pressure equipment. W0 covers the material manufacturer, W3/1 GJL, W3/2 GJS. W3/3 austenitic cast iron is not on offer. Röth is certified to AD2000 for iron castings that fit the Pressure Equipment Directive. The certificate is evidence, not a release of a given valve housing. It is not the same as ISO 9001. Conformity of the pressure device stays with the equipment manufacturer.
More … DIN EN 1561DIN EN 1563Grey iron
CertificationRequest advice
Quality
Also called: HB, HB 30, Hardness test
Brinell hardness presses a carbide ball into the surface and measures the indent. On cast iron this is the usual hardness method. The HB figure stands in the material tables as a guide value. It is not the same as tensile strength on the test bar. Anyone who converts HB into Rm and sets that as a specification does not set the inspection where it belongs.
More … Grey ironDuctile ironGJL
Materials GJL / GJSCapabilities
Materials
Also called: Iron casting, Cast-iron material
Cast iron is an iron-carbon alloy with enough carbon for graphite to form. It is poured in a mould, not rolled or forged. At Röth this means grey and ductile iron to DIN EN 1561 and DIN EN 1563, not aluminium or steel castings.
More … Grey ironDuctile ironGJL
Materials GJL / GJSRequest advice
Design
Also called: Gussbarkeit
Castability is the judgement of whether geometry, material and lot size fit the process. At Röth: green-sand machine moulding, GJL or GJS, cores, flask or mould-block size, 0.2-200 kg depending on the line. A part can be clever on the drawing and still not castable in this shop.
More … Design for castingCore-intensive castingMachine moulding
CapabilitiesRequest advice
Quality
Casting defects are deviations that arise in moulding, pouring or freezing: shrinkage, gas pores, cold shut, core shift, scab. Not every finding is scrap. What counts is the agreed inspection, location and function. Fault analysis and a complaint are two different paths. Anyone who calls every hole shrinkage picks the wrong countermeasure.
More … Shrinkage cavityCold shutScab
CapabilitiesCertification
Cores
Also called: Core supports
Chaplets are small metal pieces that support the core against lift and sag. They sit between core and mould wall. They fuse on or stay in the part. Without them a heavy or long core wanders. Röth also makes chaplets as a shop aid for other foundries.
More … Core ironsSand coreCore shift
Chaplets / core irons
Materials
Also called: Chill, Edge hardness
A chilled structure forms when carbon does not precipitate as graphite but as iron carbide. The structure becomes hard, white in the fracture and poorly machinable. Typical on thin walls, edges and next to a metal chill when cooling is too sharp.
More … ChillsInoculationWall thickness
Materials GJL / GJSChills
Cores
Also called: Chill insert, Chill
A chill is a metal piece in the mould or on the core that takes heat away locally. It is meant to freeze a hotspot faster and avoid shrinkage. If it sits too sharply against a thin wall, a chilled structure is a risk. Röth uses chills in its own work and supplies them as a shop aid to other foundries.
More … HotspotChilled structureSolidification simulation
ChillsCapabilities
Quality
Also called: Misrun
A cold shut forms when two melt fronts meet and no longer weld. The spot stays as a seam, a notch or a leaking wall. Cause is often too low a temperature, too long a flow path or too thin a wall. The skin is already too firm. It looks like a glue joint, but it is casting.
More … Casting defectGatingWall thickness
Capabilities
Cores
A core assembly is several cores built into one inside form. Housings with channels, pockets and bearing bores often need more than one core. The assembly must sit in the mould, hold against lift and still come apart after the pour. Each joint between the cores is a possible shift line.
More … Sand coreCore printCore-intensive casting
CapabilitiesRapid prototyping
Cores
Also called: Core reinforcement
Core iron is a metal insert in the sand core. It keeps the core stiff so it does not break or sag when set or under lift. After the pour the iron stays in the part or comes out with the core, depending on where it sits. Röth also supplies core irons as a shop aid for other foundries.
More … ChapletsSand coreChills
Chaplets / core irons
Cores
Also called: Core prints
The core print is the seat for the core in the mould. It sets position and often the seal against incoming melt. The pattern carries the print, the core box the counterpart. Too tight, and the core shifts. Too loose, and iron runs into the print or the core floats.
More … Sand coreCore shiftCore assembly
CapabilitiesRequest advice
Cores
Also called: Core displacement
Core shift means the core has moved, tipped or floated. The inner contour then sits beside the outer contour. Wall thicknesses tip, bores wander. Cause is the print, lift, setting or a core that is too weak. The iron is there. It is just in the wrong place.
More … Core printSand coreCasting defect
CapabilitiesChaplets / core irons
Cores
Also called: core-intensive, core-intensive housings
Core-intensive casting means parts whose inside sets the work: many cores, an assembly, tight channels, undercuts. That is the main work at Röth, not the simple solid lump. Machine moulding does not change that. The machine moulds the outside, the cores stay craft and setting.
More … Sand coreCore assemblyMachine moulding
CapabilitiesRequest advice
Quality
Also called: Flash rust, VCI
Corrosion protection on a raw casting here means storage and transport, not a paint line. Unmachined cast iron rusts in air and moisture. VCI film, dry storage and short routes keep flash rust small. The protection does not replace an agreed coating at the customer. Flash rust is not the same as deeper storage rust.
More … Raw castingGrey ironFettling
CapabilitiesRequest advice
Design
Also called: designed for casting, casting-friendly design
Castable design takes account of parting, draft, cores, wall thicknesses and feeding before the pattern is built. It cuts shrinkage, shift and rework. It does not make the part ugly. It makes it producible in sand and in series.
More … CastabilityDraftWall thickness
CapabilitiesRequest advice
Standards
DIN EN 1561 is the standard for flake-graphite cast iron, that is grey iron. It sets grades, designations and characteristic values. The short marks are EN-GJL. The table values on the Röth materials page are guide values. The standard text remains binding. At Röth sit EN-GJL-150, 200, 250 and 300. GG-20 sits with EN-GJL-200, GG-25 with EN-GJL-250. Anyone who writes GG-25 and expects EN-GJL-300 mixes two languages.
More … Grey ironGJLDIN EN 1563
Materials GJL / GJSCertification
Standards
DIN EN 1563 is the standard for spheroidal-graphite cast iron, that is ductile iron. The short marks are EN-GJS, with strength and elongation in the designation. At Röth the grades carried sit in a table: EN-GJS-400-15, 400-18-LT, 500-7, 600-3, 700-2 and 500-14. The standard text remains binding. The website table is a guide value.
More … Ductile ironGJSDIN EN 1561
Materials GJL / GJSCertification
Moulding
Also called: Pattern draft, Withdrawal taper
Draft is a slight taper on walls that stand perpendicular to the joint. Without it the pattern sticks in the sand or tears the mould on withdrawal. Inner faces formed by a core often need a different logic than the outer mould. The taper belongs in the raw casting, not first in machining. The drawing names the angle in degrees once the joint is fixed.
More … Design for castingUndercutCastability
CapabilitiesRequest advice
Materials
Also called: Spheroidal graphite iron, Ductile iron GJS
Ductile iron is cast iron in which the graphite is spheroidal. The spheroids notch the matrix less than flakes. Strength and elongation sit closer to steel. The grades are called GJS and sit in DIN EN 1563.
More … GJSSpheroidal graphiteMagnesium treatment
Materials GJL / GJSRequest advice
Moulding
Also called: Feeding, Feeder practice
A feeder is an extra volume of melt that stays liquid longer than the critical spot in the part. It compensates solidification shrinkage and should prevent shrinkage cavities. It must be connected to the hotspot and solidify later than that. After the pour it is fettled off. Position and size come from the feeding layout, often with simulation.
More … Shrinkage cavityShrinkageGating
Capabilities
Moulding
Fettling removes gating, feeders, flash and adhering moulding sand. After that the part is often blasted. Only then is the raw casting ready to ship. Fettling is work on the part, not the machining of the functional faces. The fettling mark stays a casting scar until someone mills. Separation comes before blasting. The other way round one makes a lump of the feeder and dust of slag on the part.
More … Raw castingGatingFeeder
CapabilitiesRequest advice
Materials
Flake graphite is thin, irregular graphite plates in cast iron. They make grey iron brittle and give it damping and thermal conductivity. In the standard family the material is called GJL.
More … Grey ironSpheroidal graphiteCast iron
Materials GJL / GJS
Moulding
Also called: Flask mould, HWS moulding line
Flask moulding forms cope and drag in a frame. The flask size limits length, width and height of the part. At Röth that is the HWS line at 1030×810×320/320 mm by the SEIATSU process, piece weight 5-200 kg. The counterpart is flaskless moulding without a flask. The frame carries the mould to the pouring line. Without it a soft sand block breaks in the row.
More … SEIATSUMachine mouldingFlaskless moulding
CapabilitiesRequest advice
Moulding
Also called: Disamatic, Mould block
Flaskless moulding forms without a flask. The machine presses sand into a mould block with two mould halves. At Röth that is the Disamatic with mould block 600×480×150-395 mm, piece weight 0.2-30 kg, suitable from about 20 moulds per lot. The counterpart is flask moulding on the HWS. The joint stands vertical. Gating and core position turn with it.
More … Flask mouldingMachine mouldingGreen sand
CapabilitiesRequest advice
Moulding
Also called: Gating system, Ingate
Gating is the channel system from the sprue to the mould cavity. It fills the part, controls speed and should not carry slag and air into the component. Sprue, runner and ingates sit in a section ratio. Together with the feeders it belongs to the foundry layout, not to the finished-size drawing. After the pour it is fettled off. On the finished part at most the scar remains.
More … FeederSand castingSolidification simulation
Capabilities
Materials
Also called: EN-GJL, GJL-250
GJL is the designation for cast iron with flake graphite. It replaces older names such as GG. After GJL comes the grade, for example EN-GJL-250 for a tensile strength of at least 250 N/mm² on the test bar to DIN EN 1561. The flakes damp and conduct heat. The number applies first to the bar.
More … Grey ironDIN EN 1561GJS
Materials GJL / GJSRequest advice
Materials
Also called: EN-GJS, GGG, GJS-400-15
GJS is the designation for cast iron with spheroidal graphite. Older drawings write GGG. After GJS come strength and elongation, for example EN-GJS-400-15: at least 400 N/mm² tensile strength and 15 percent elongation on the test bar to DIN EN 1563. Without magnesium treatment after desulphurisation the flake stays.
More … Ductile ironDIN EN 1563GJL
Materials GJL / GJSRequest advice
Moulding
Also called: Green-sand moulding
Green sand is moulding sand bonded with bentonite and water and going into the mould moist. Green here is not the colour and not environmentally friendly, but: the mould is not baked before pouring. Green-sand moulding sand is the same word. That is the moulding material of the machine moulding lines at Röth. Bentonite is a clay mineral, not a colourant and not an eco-balance.
More … Moulding materialSand castingMachine moulding
CapabilitiesRequest advice
Materials
Also called: Grey cast iron, Grey-iron
Grey iron is cast iron in which the graphite is present as flakes. The material is brittle, conducts heat well and damps vibration. The grades are called GJL and sit in DIN EN 1561. At Röth those are EN-GJL-150, 200, 250 and 300.
More … GJLFlake graphiteDIN EN 1561
Materials GJL / GJSRequest advice
Moulding
In hand moulding the moulder compacts the sand by hand or with hand tools around a pattern. The mould is free in size, the cycle is slow. Machine moulding reverses that: fixed mould size, high cycle. Röth produces on moulding lines, not as a classic hand-moulding shop. Large one-offs outside the machine sizes are not in the offer. The contrast explains the limit, it does not describe a second hall in Mosbach.
More … Machine mouldingSand castingMoulding material
CapabilitiesRequest advice
Materials
Also called: Heat concentration, Metal accumulation
A hotspot is a spot in the casting that stays liquid longer than the surroundings. Usually a metal accumulation, a boss junction or a sharp wall transition. Shrinkage cavities and a coarse structure threaten in the node if nobody feeds or cools. The thin edge beside it can chill (white iron / carbide); that is a second defect at the same place, not the hotspot itself.
More … Shrinkage cavityChillsSolidification simulation
CapabilitiesChills
Materials
Also called: Inoculated iron, Melt inoculation
Inoculation is the addition of an inoculant to the melt shortly before pouring. It supplies nuclei on which graphite can grow. Without inoculation there is a risk of undercooling, a coarse structure or chill, especially in thin sections.
More … Cast ironChilled structureGrey iron
Materials GJL / GJSCapabilities
Moulding
Also called: Machine moulding shop
Machine moulding compacts the moulding sand on a moulding line. The mould is made in cycle, with a fixed flask size or as a mould block. The counterpart is hand moulding, where the mould is compacted by hand. At Röth, HWS and Disamatic run in green sand. The machine moulds the outside. The cores form the inside. Repeatability sits in plate, sand window and cycle, not in the craft of a single moulder.
More … Hand mouldingGreen sandFlask moulding
CapabilitiesRequest advice
Design
Also called: Stock, Machining stock
Machining allowance is material above the finished size so turning and milling find a clean face. Too little, and the skin or the shift stays. Too much, and machining eats time. The allowance belongs in the pattern, not in hope on the bench.
More … Raw castingShrinkageDesign for casting
CapabilitiesCasting tolerance checkRequest advice
Materials
Also called: Mg treatment
Magnesium treatment puts magnesium into the desulphurised melt. The graphite then grows spheroidal instead of flaky. Without this step there is no ductile iron, whatever the drawing says. Inoculation follows. Magnesium forms the spheroid. Inoculation supplies the nuclei.
More … Ductile ironSpheroidal graphiteInoculation
Materials GJL / GJS
Moulding
Also called: Moulding sand
Moulding material is the mix the sand mould is made from. For the outer mould at Röth that is green sand: silica sand, bentonite, water. Cores use other binders. Preparation and sand testing keep the moulding material in the window. Moulding material is the sand, the material is the iron. Both in one sentence mix mould and melt.
More … Green sandSand castingFettling
CapabilitiesRequest advice
Prototype
Rapid prototyping here means: a grey or ductile iron casting in a short time, without already building the later series pattern equipment. At Röth this runs via 3D sand printing of the mould or the cores. The aim is a checkable raw part, often in 15-25 working days with STP, not a plastic sample. The iron is GJL or GJS. After that series can switch to HWS or Disamatic.
More … 3D sand printingSand castingDesign for casting
Rapid prototypingCapabilities
Moulding
Also called: As-cast part, Raw castings
The raw casting is the casting the foundry delivers: fettled, often blasted, with allowance on the machining faces. It is not yet the finished part from machining. Dimensional accuracy here means the raw casting plus the agreed allowance, not the finished size on the drawing. Gating and feeders are off. Function comes after that. Röth delivers iron in this condition. The customer machines.
More … FettlingMachining allowanceCast iron
CapabilitiesCasting tolerance checkRequest advice
Moulding
Also called: Sand moulding
Sand casting means: the mould is sand, not a permanent metal mould. The sand takes the geometry from the pattern or from the printed core package. After the pour the mould is destroyed. Bentonite-bonded green sand, chemically hardened sand and vacuum-bonded moulds belong to the same family. Machine moulding and hand moulding are ways of making this mould. Outer mould and core are both sand, but rarely the same mix.
More … Green sandMachine mouldingMoulding material
CapabilitiesRequest advice
Cores
Also called: Core, Cores
A sand core is a shaped sand body set into the mould. Where the core sits, the iron stays hollow. Without cores there would be no internal channels, pockets or bearing bores in the raw part. The core is made in a core box or in sand printing, hardens and carries the inner contour. At Röth, cores are the rule, not the exception.
More … Core assemblyCore printCore-intensive casting
CapabilitiesRapid prototyping
Quality
A scab is a layer of moulding sand that comes off the mould and falls into the melt or sticks to the part. The surface then carries a scale, a scar or trapped sand. Cause often sits in the moulding material, in compaction or in the flow on fill. Scale and a fettling mark look similar if you do not look.
More … Casting defectMoulding materialGreen sand
Capabilities
Moulding
Also called: SEIATSU process, Air-flow squeeze moulding
SEIATSU is an air-flow squeeze moulding process. First air flows through the moulding sand, then the squeeze follows. The aim is even compaction in the flask. At Röth the HWS moulding line works by this process. SEIATSU is a moulding process, not an alloy and not a certificate. It does not sit beside EN-GJL-250 on the drawing and not as a grade on the delivery note.
More … Flask mouldingGreen sandMachine moulding
CapabilitiesRequest advice
Materials
Also called: Shrinkage allowance, Volume shrinkage
Shrinkage is the volume loss when the melt solidifies and the part cools to room temperature. Without compensation, shrinkage cavities form or the raw casting is undersize. Compensation is feeders, gating and the allowance in the pattern.
More … FeederShrinkage cavityMachining allowance
CapabilitiesRequest advice
Materials
Also called: Lunker, Solidification shrinkage
A shrinkage cavity is a void that forms when melt solidifies and nobody feeds the volume loss. It often sits in the hotspot: in metal accumulations, bosses and wall transitions. Inspection finds it, feeding and simulation should prevent it beforehand.
More … HotspotFeederSolidification simulation
CapabilitiesRequest advice
Quality
Also called: MAGMA, MAGMA simulation, Casting simulation
Solidification simulation calculates fill, temperature and solidification on the 3D model before the first mould is built. It shows hotspots, possible shrinkage and poor flow paths. At Röth this has run since 2008 with MAGMA, as part of the layout. The calculation sits before the first pour: it does not pour, it does not inspect the heat and it does not inspect the finished part.
More … Shrinkage cavityHotspotFeeder
CapabilitiesRequest advice
Materials
Also called: EN-GJS-500-14, Solution-strengthened ferritic cast iron
Solution-strengthened ferritic iron here means ferritic iron with spheroidal graphite, in which a high silicon content in the matrix raises strength. The grade at Röth is EN-GJS-500-14. Hardness and strength sit closer together than in ferritic-pearlitic grades. The values apply to the test bar, not automatically to every wall in the housing.
More … Ductile ironGJSDIN EN 1563
Materials GJL / GJSRequest advice
Quality
Spectro analysis measures the chemical composition of the melt. Carbon, silicon, manganese, sulphur, phosphorus and the other companions must fit the grade. Without this measurement GJL or GJS stays a name on the order. The analysis says what is in the ladle. It does not say how the melt freezes and not what sits in the housing.
More … Thermal analysisCast ironGJL
CapabilitiesMaterials GJL / GJS
Materials
Also called: Spherulitic graphite, Nodular graphite
Spheroidal graphite is nearly round graphite particles in cast iron. They notch the matrix less than flakes. That is why ductile iron carries higher loads and elongates more. The form comes from magnesium treatment of the melt, after desulphurisation. Without that step the flake stays.
More … Ductile ironMagnesium treatmentFlake graphite
Materials GJL / GJS
Materials
Also called: Annealing, Stress-relief annealing of cast iron
Stress-relief annealing is a heat treatment that reduces residual stresses in the casting without rebuilding the structure from the ground up. The part is held and cooled slowly. Soft annealing and pearlite annealing are other anneals with a different aim.
More … Cast ironShrinkageGrey iron
Materials GJL / GJSRequest advice
Quality
Thermal analysis records the cooling curve of a melt sample. From the arrests the foundry reads how the melt freezes: graphite, undercooling, tendency to chill. It complements spectro analysis, it does not replace it. The curve applies to the sample in the cup. It does not apply to every hotspot in the housing.
More … Spectrographic analysisInoculationChilled structure
Capabilities
Design
An undercut is a shape that blocks the pattern or the core in the parting direction. Outside, a core or another parting frees it. Inside, it often takes a split core assembly. With no solution the mould sticks or the part has no cavity.
More … Sand coreDraftDesign for casting
CapabilitiesRequest advice
Design
Also called: Section thickness
Wall thickness decides how fast a spot freezes. Thick stays liquid longer, thin chills off. Jumps with no radius build hotspots. In iron casting, minimum wall, transition and tie-in to bosses belong together, not the thinnest wall alone.
More … HotspotChilled structureDesign for casting
CapabilitiesRequest advice
No entries for this filter.