Grey and ductile iron grades

Grey iron, ductile iron and special alloys. Characteristic data, standards and properties.

DIN EN 1561

Grey iron

  • Thermal conductivity
  • Damping
  • Cost efficiency

Grey iron is an iron-carbon alloy with at least 2% carbon, usually 2 to 4%. Graphite sits as thin, irregular flakes. The material is brittle, conducts heat well and damps vibration. The designation is GJL.

Note: Guide values from separately cast test bars. The lower tensile figure is the DIN EN 1561 grade minimum; the span is typical and informative. Elongation 0.3–0.8% is a shared guide band, not a grade-by-grade DIN figure. Density, fracture toughness, resistivity and compressive, bending, shear and fatigue strength are physical guides, not bar-acceptance values. Castings may differ with geometry and production. Binding remains DIN EN 1561.

Request advice on Grey iron
Grey-iron gearbox housing, typical application
Specifications Grey iron
Material name EN-GJL-150EN-GJL-200EN-GJL-250EN-GJL-300
Tensile strength Rm [N/mm²] min. 150, typically up to 250min. 200, typically up to 300min. 250, typically up to 350min. 300, typically up to 400
0.1% proof strength Rp0.1 [N/mm²] 98 – 165130 – 195165 – 228195 – 260
Elongation A [%] 0,3 – 0,80,3 – 0,80,3 – 0,80,3 – 0,8
Brinell hardness HB 30 125 – 205150 – 230180 – 250200 – 275
Modulus of elasticity [kN/mm²] 78 – 10388 – 113103 – 118108 – 137
Compressive strength [N/mm²] 600720840960
Bending strength [N/mm²] 250290340390
Shear strength [N/mm²] 170230290345
Poisson’s ratio 0,260,260,260,26
Bending fatigue strength [N/mm²] 7090120140
Tension-compression fatigue strength [N/mm²] 40506075
Fracture toughness KIc [N/mm³/²] 320400480560
Density [g/cm³] 7,107,157,207,25
Electrical resistivity [Ω·mm²/m] 0,800,770,730,70

EN-GJL-150

Tensile strength Rm [N/mm²]
min. 150, typically up to 250
0.1% proof strength Rp0.1 [N/mm²]
98 – 165
Elongation A [%]
0,3 – 0,8
Brinell hardness HB 30
125 – 205
Modulus of elasticity [kN/mm²]
78 – 103
Compressive strength [N/mm²]
600
Bending strength [N/mm²]
250
Shear strength [N/mm²]
170
Poisson’s ratio
0,26
Bending fatigue strength [N/mm²]
70
Tension-compression fatigue strength [N/mm²]
40
Fracture toughness KIc [N/mm³/²]
320
Density [g/cm³]
7,10
Electrical resistivity [Ω·mm²/m]
0,80

EN-GJL-200

Tensile strength Rm [N/mm²]
min. 200, typically up to 300
0.1% proof strength Rp0.1 [N/mm²]
130 – 195
Elongation A [%]
0,3 – 0,8
Brinell hardness HB 30
150 – 230
Modulus of elasticity [kN/mm²]
88 – 113
Compressive strength [N/mm²]
720
Bending strength [N/mm²]
290
Shear strength [N/mm²]
230
Poisson’s ratio
0,26
Bending fatigue strength [N/mm²]
90
Tension-compression fatigue strength [N/mm²]
50
Fracture toughness KIc [N/mm³/²]
400
Density [g/cm³]
7,15
Electrical resistivity [Ω·mm²/m]
0,77

EN-GJL-250

Tensile strength Rm [N/mm²]
min. 250, typically up to 350
0.1% proof strength Rp0.1 [N/mm²]
165 – 228
Elongation A [%]
0,3 – 0,8
Brinell hardness HB 30
180 – 250
Modulus of elasticity [kN/mm²]
103 – 118
Compressive strength [N/mm²]
840
Bending strength [N/mm²]
340
Shear strength [N/mm²]
290
Poisson’s ratio
0,26
Bending fatigue strength [N/mm²]
120
Tension-compression fatigue strength [N/mm²]
60
Fracture toughness KIc [N/mm³/²]
480
Density [g/cm³]
7,20
Electrical resistivity [Ω·mm²/m]
0,73

EN-GJL-300

Tensile strength Rm [N/mm²]
min. 300, typically up to 400
0.1% proof strength Rp0.1 [N/mm²]
195 – 260
Elongation A [%]
0,3 – 0,8
Brinell hardness HB 30
200 – 275
Modulus of elasticity [kN/mm²]
108 – 137
Compressive strength [N/mm²]
960
Bending strength [N/mm²]
390
Shear strength [N/mm²]
345
Poisson’s ratio
0,26
Bending fatigue strength [N/mm²]
140
Tension-compression fatigue strength [N/mm²]
75
Fracture toughness KIc [N/mm³/²]
560
Density [g/cm³]
7,25
Electrical resistivity [Ω·mm²/m]
0,70
DIN EN 1563

Ductile iron

  • High strength
  • Closer to steel than grey iron
  • Wide industrial use

Ductile iron is an iron-carbon alloy with spheroidal graphite. The sphere comes from magnesium treatment after desulphurisation, not from magnesium alone. Inoculation follows. Strength and elongation sit closer to steel than in grey iron. The designation is GJS.

Note: Guide values from separately cast test bars. Tensile strength and elongation are DIN EN 1563 grade minima. Density is informative; high-carbon GJS can sit below 7.00 g/cm³. Shear strength is a table figure, not a bar-acceptance value. Castings may differ with geometry and production. Binding remains DIN EN 1563.

Request advice on Ductile iron
Ductile-iron gearbox housing, typical application
Specifications Ductile iron
Material name EN-GJS-400-15EN-GJS-400-18-LTEN-GJS-500-7EN-GJS-600-3EN-GJS-700-2
Tensile strength Rm [N/mm²] min. 400min. 400min. 500min. 600min. 700
0.2% proof strength [N/mm²] 250240320370420
Elongation A [%] 1518732
Brinell hardness HB 30 135 – 180130 – 175150 – 220190 – 270225 – 305
Modulus of elasticity [kN/mm²] 169169165 – 175174176
Shear strength [N/mm²] 360360450540630
Density [g/cm³] 7,107,107,207,207,20
Charpy impact energy at −20 °C [J] 12

EN-GJS-400-15

Tensile strength Rm [N/mm²]
min. 400
0.2% proof strength [N/mm²]
250
Elongation A [%]
15
Brinell hardness HB 30
135 – 180
Modulus of elasticity [kN/mm²]
169
Shear strength [N/mm²]
360
Density [g/cm³]
7,10

EN-GJS-400-18-LT

Tensile strength Rm [N/mm²]
min. 400
0.2% proof strength [N/mm²]
240
Elongation A [%]
18
Brinell hardness HB 30
130 – 175
Modulus of elasticity [kN/mm²]
169
Shear strength [N/mm²]
360
Density [g/cm³]
7,10
Charpy impact energy at −20 °C [J]
12

EN-GJS-500-7

Tensile strength Rm [N/mm²]
min. 500
0.2% proof strength [N/mm²]
320
Elongation A [%]
7
Brinell hardness HB 30
150 – 220
Modulus of elasticity [kN/mm²]
165 – 175
Shear strength [N/mm²]
450
Density [g/cm³]
7,20

EN-GJS-600-3

Tensile strength Rm [N/mm²]
min. 600
0.2% proof strength [N/mm²]
370
Elongation A [%]
3
Brinell hardness HB 30
190 – 270
Modulus of elasticity [kN/mm²]
174
Shear strength [N/mm²]
540
Density [g/cm³]
7,20

EN-GJS-700-2

Tensile strength Rm [N/mm²]
min. 700
0.2% proof strength [N/mm²]
420
Elongation A [%]
2
Brinell hardness HB 30
225 – 305
Modulus of elasticity [kN/mm²]
176
Shear strength [N/mm²]
630
Density [g/cm³]
7,20

Solution-strengthened ferritic cast iron

(high-silicon spheroidal graphite iron)

  • Uniform hardness
  • Improved machinability
  • High elongation

Unlike ferritic/pearlitic grades, solution-strengthened ferritic grades with a spheroidal graphite matrix are single-phase, so hardness scatter is smaller.

At a similar hardness, the smaller scatter and lower pearlite content improve machinability.

Combining high strength with a very high minimum elongation for cast iron opens new design options.

The mechanical properties of solution-strengthened ferritic iron fall in a narrower range and are more uniform throughout the casting. Benefits are uniform machined surfaces and wall-thickness optimisation.

Note: Guide values from separately cast test bars. Tensile strength and elongation are DIN EN 1563 grade minima. The 80 J unnotched at 23 °C is a table figure, not a DIN acceptance value; notched energy often sits at a few joules, as for 500-7. High elongation is not impact toughness. Castings may differ with geometry and production. Binding remains DIN EN 1563.

Request advice on Solution-strengthened ferritic cast iron
Solution-strengthened ferritic cast-iron casting
Specifications Solution-strengthened ferritic cast iron
Material EN-GJS-500-14
Tensile strength Rm [N/mm²] min. 500
0.2% proof strength [N/mm²] 400
Elongation A [%] 14
Brinell hardness HB 30 185 – 215
Modulus of elasticity [kN/mm²] 170
Unnotched impact energy at 23 °C [J], informative 80

EN-GJS-500-14

Tensile strength Rm [N/mm²]
min. 500
0.2% proof strength [N/mm²]
400
Elongation A [%]
14
Brinell hardness HB 30
185 – 215
Modulus of elasticity [kN/mm²]
170
Unnotched impact energy at 23 °C [J], informative
80